title: "Yield Strength vs Tensile Strength: What to Design To"
description: "Yield strength vs tensile strength: the stress-strain curve, 0.2% offset yield, elongation, spec minimums for common alloys, and what to put on an RFQ."
canonical: https://openspindle.com/blog/yield-strength-vs-tensile-strength
author: "Tom"
datePublished: 2026-11-12T17:00:00.000Z
dateModified: 2026-11-12T17:00:00.000Z
category: "Materials"
---

# Yield Strength vs Tensile Strength: Which Number to Design To

Yield strength is the stress at which a metal starts to deform permanently, usually measured at 0.2 percent offset strain. Ultimate tensile strength (UTS) is the highest stress it carries before it necks and breaks. Parts are designed to yield divided by a safety factor, because a part that has yielded is bent even if it has not broken. UTS and elongation tell you how much margin and ductility sit beyond that point.

## The stress-strain curve in one paragraph

A tensile test (ASTM E8/E8M for metals) pulls a machined test bar at a controlled rate and records load against stretch. Divide load by the original cross-section and you get stress; divide the stretch by the original gauge length and you get strain. Plot one against the other and every ductile metal draws roughly the same shape.

- **Elastic region.** A straight line from the origin. Unload anywhere on it and the bar returns to its original length. The slope is the elastic modulus (stiffness).
- **Yield.** The line starts to curve. From here on, some of the stretch is permanent.
- **Strain hardening.** The curve keeps climbing as the metal work hardens, but more slowly.
- **Ultimate tensile strength.** The peak of the curve. The bar starts to neck down at one spot.
- **Fracture.** The necked section thins until it breaks. The permanent stretch measured after the pieces are fitted back together is the elongation.

Yield strength, UTS and elongation are the three numbers a mill reports, and each one answers a different design question.

## Yield strength and the 0.2 percent offset

Most aluminum, stainless and titanium alloys have no sharp point where yielding starts. The curve bends gradually. To get a repeatable number, the test standard draws a line parallel to the elastic slope, offset by 0.002 strain (0.2 percent), and reports the stress where that line crosses the curve. That is the 0.2 percent offset yield strength, sometimes written Rp0.2 in ISO and EN documents.

In plain terms, it is the stress that leaves the part about 0.2 percent longer after you unload it. On a 100 mm bracket arm that is 0.2 mm of permanent set, which is already enough to throw a precision assembly out of alignment.

Some low-carbon steels such as A36 and 1018 show a distinct yield point: the load drops slightly, then the bar stretches at nearly constant load before hardening resumes. Their certs may report an upper or lower yield point instead of an offset value. For design purposes, treat either as the yield strength the spec guarantees.

## Ultimate tensile strength and elongation

UTS is the maximum load divided by the original cross-section. It is the number that tells you when a part breaks, not when it bends, so it matters for fasteners, burst and crash cases, and anything where a one-time overload must not separate.

The gap between yield and UTS is useful information. The ratio of yield to UTS runs from roughly 0.4 for annealed 304 stainless to above 0.9 for some heat-treated alloys. A low ratio means the metal has a lot of strain-hardening margin after it yields and gives plenty of visible warning. A ratio close to 1 means there is little room between permanent bending and fracture.

Elongation is the permanent stretch at fracture as a percentage of the gauge length, usually 2 in or 50 mm (some specs use 4D or 5D gauge lengths, so compare like with like). It is the closest single number to ductility. It predicts, loosely, how a metal tolerates bending, forming, crimping and impact. A 7075-T6 plate with about 11 percent elongation and annealed 304 at 40 percent or more both pass their specs, but they behave very differently in a press brake.

One phrase worth clearing up: "ultimate yield strength" is not a property. People who search for it usually want ultimate tensile strength, sometimes yield strength. If you see it on a drawing, ask which one the designer meant.

## Typical minimum values for common alloys

These are specification minimums or, where the common product spec sets none, typical published values. Mill certs for real heats usually come in above the minimum, but you design to the minimum because that is all the spec guarantees.

| Alloy and condition | Yield, min | UTS, min | Elongation, min | Basis |
| --- | --- | --- | --- | --- |
| Aluminum 6061-T6 / T651 sheet and plate | 240 MPa (35 ksi) | 290 MPa (42 ksi) | About 8 to 10% | ASTM B209, varies by thickness |
| Aluminum 7075-T6 / T651 sheet and plate | About 434 to 476 MPa (63 to 69 ksi) | About 510 to 538 MPa (74 to 78 ksi) | About 7 to 9% | ASTM B209, varies by thickness |
| Aluminum 5052-H32 sheet | 160 MPa (23 ksi) | 215 MPa (31 ksi) | About 7 to 12% | ASTM B209, varies by thickness |
| Steel A36 plate and shapes | 250 MPa (36 ksi) | 400 to 550 MPa (58 to 80 ksi) range | 20% in 8 in, 23% in 2 in | ASTM A36 |
| Steel 1018 cold drawn bar | About 370 MPa (54 ksi) typical | About 440 MPa (64 ksi) typical | About 15% typical | Typical (MatWeb); ASTM A108 sets no tensile minimum unless ordered |
| Alloy steel 4140 annealed | About 415 MPa (60 ksi) typical | About 655 MPa (95 ksi) typical | About 25% typical | Typical (MatWeb) |
| Alloy steel 4140 quenched and tempered | 720 MPa (105 ksi) | 860 MPa (125 ksi) | 16% | ASTM A193 Grade B7, up to 2.5 in |
| Stainless 304 annealed | 205 MPa (30 ksi) | 515 MPa (75 ksi) | 40% | ASTM A240 |
| Stainless 316 annealed | 205 MPa (30 ksi) | 515 MPa (75 ksi) | 40% | ASTM A240 |
| Stainless 17-4 PH, H1025 | 1000 MPa (145 ksi) | 1070 MPa (155 ksi) | 12% | ASTM A564 |
| Stainless 17-4 PH, H900 | 1170 MPa (170 ksi) | 1310 MPa (190 ksi) | 10% | ASTM A564 |
| Titanium Ti-6Al-4V (Grade 5) annealed bar | 828 MPa (120 ksi) | 895 MPa (130 ksi) | 10% | ASTM B348 |

*Minimums depend on product form, thickness and test direction, and the governing spec edition. Use the spec your drawing calls out, not this table, for any part where margin is tight. Typical 6061-T6 values (276 MPa yield, 310 MPa UTS) appear in many charts and run about 15 percent above the B209 minimum.*

## Why designs use yield and a safety factor

Most mechanical parts fail functionally long before they break. A shaft that has taken a permanent set wobbles, a bracket that has bent misaligns whatever it holds, a bolted joint that has yielded loses clamp load. So the usual static check is: working stress must stay below yield strength divided by a safety factor.

The factor covers what you do not know: load uncertainty, stress concentrations at holes and corners, material scatter, and the gap between a calculation and a real part. For well-understood static loads, factors of roughly 1.5 to 3 on yield are common. Uncertain loads, shock, or human safety push that higher, and industry codes (pressure vessels, structural steel, aerospace, lifting equipment) set their own factors that override any rule of thumb.

Two cases where yield is not the governing number:

- **Fatigue.** Parts that see millions of load cycles fail at stresses well below yield. Aluminum has no true endurance limit, so cyclic aluminum parts are sized to a fatigue strength at a stated cycle count, not to yield.
- **Welded aluminum.** Welding 6061-T6 anneals the heat-affected zone. AWS D1.2 uses a minimum as-welded tensile strength of 24 ksi (165 MPa) for 6061-T6, against 42 ksi for the unwelded sheet. If the part is welded, the cert value for the parent metal is not the strength at the weld.

## Where these numbers show up on a mill test report

A [mill test report](/blog/mill-test-report) lists the mechanical test results for the heat or lot your material came from, normally in a block labeled tensile, yield, elongation and sometimes reduction of area and hardness. Read three things:

- **Units and basis.** Yield may be listed in ksi or MPa, as 0.2 percent offset or as a yield point. Elongation should state the gauge length.
- **The spec it was tested to.** The cert should name the same spec and temper your drawing calls out, for example ASTM B209 6061-T651. A cert for 6061-T6 bar does not certify T651 plate.
- **Test direction.** Plate and sheet are often tested in the long transverse direction. Properties through the thickness of thick plate can run lower.

The cert value is for a test coupon from that heat, not for your finished part. If your part is heat treated, welded or heavily cold worked after it leaves the mill, the cert no longer describes it, and you need a test or a hardness check after processing if strength matters.

## What to specify on a drawing or RFQ

A strength number on its own is a weak callout. A shop cannot buy "steel with 50 ksi yield" off the shelf without guessing an alloy. Specify the material the way it is sold and the strength follows from the spec.

- **Alloy, temper or condition, and spec.** For example: 6061-T6 per ASTM B209, A36 per ASTM A36, 304 annealed per ASTM A240, 17-4 PH per AMS 5643 heat treated to H1025.
- **Certs if you need them.** Ask for a mill test report (or EN 10204 3.1 certificate) when the part is load-bearing, regulated or traceable. Asking on the RFQ costs little; asking after material is cut can mean new stock.
- **A minimum property only when it is the real requirement.** If the design needs a minimum yield above the spec minimum, write it as an extra requirement (for example: minimum yield 45 ksi, verify on cert) and expect it to narrow the stock a shop can use.
- **Post-processing strength.** If you heat treat after machining, give the heat treatment and the hardness or strength to verify, not just the starting temper.

For a side-by-side of density, hardness and strength across the common machining metals, see the [metal properties comparison chart](/reference/metal-properties-comparison).

## Related reading

- [Metal properties comparison chart](https://openspindle.com/reference/metal-properties-comparison.md)
- [How to read a mill test report](https://openspindle.com/blog/mill-test-report.md)
- [Material certifications explained](https://openspindle.com/blog/material-certifications-explained.md)
- [Hardness conversion chart](https://openspindle.com/reference/hardness-conversion-chart.md)
- [How to write an RFQ](https://openspindle.com/blog/how-to-write-an-rfq.md)

## Frequently asked questions

### What is the difference between yield strength and tensile strength?

Yield strength is the stress where a metal starts to deform permanently, usually defined at 0.2 percent offset strain. Tensile strength, or ultimate tensile strength, is the highest stress the metal carries before it necks and fractures. Yield tells you when a part bends for good; tensile strength tells you when it breaks.

### Is ultimate yield strength the same as ultimate tensile strength?

"Ultimate yield strength" is not a standard property. It is a mix of two terms. In most cases the person means ultimate tensile strength (the peak of the stress-strain curve); sometimes they mean yield strength. If it appears on a drawing, ask which one was intended.

### Why do engineers design to yield strength instead of tensile strength?

Because most parts stop working once they bend permanently, well before they break. Designing to yield divided by a safety factor keeps the part in its elastic range. Tensile strength still matters for overload, burst and fastener cases, and fatigue or welding can make other limits govern.

### What does the 0.2 percent offset mean?

Many alloys have no sharp yield point, so the test standard draws a line parallel to the elastic part of the curve, shifted by 0.002 strain, and reports the stress where it crosses the curve. That stress leaves about 0.2 percent permanent stretch after unloading.

### Is a higher tensile strength always better?

No. Higher-strength tempers and alloys usually have lower elongation, so they bend less before cracking, can be harder to form and weld, and may be more notch sensitive. 6061-T6 is stronger than 5052-H32 but cracks at bend radii 5052 forms easily. Pick the strength the load needs, then check ductility for the process.

### Should I put a yield strength number on my RFQ?

Put the alloy, temper and governing spec first, because that defines the guaranteed strength. Add a minimum yield only when the design needs more than the spec guarantees, and ask for a mill test report if you need proof.