title: "Galvanic Corrosion Chart: Galvanic Series and Metal Pairs"
description: "Galvanic corrosion chart: the galvanic series in seawater, safe potential differences, common metal pairs like aluminum and stainless, and how to prevent it."
canonical: https://openspindle.com/reference/galvanic-corrosion-chart
---

# Galvanic Corrosion Chart

The galvanic series in seawater, allowable potential differences by environment, the metal pairs that fail in real assemblies, and the fixes: isolation, sealing, fastener choice and finish.

Galvanic corrosion is the accelerated corrosion of one metal when it touches a more cathodic metal and an electrolyte such as salt water or condensation bridges the two. The galvanic series ranks metals from anodic (magnesium, zinc, aluminum) to cathodic (titanium, passive stainless, graphite and carbon fiber); the farther apart two metals sit, the stronger the drive to corrode the anodic one. Prevention means breaking the circuit: choose compatible metals, isolate the joint, keep water out, and coat the cathode.

## How galvanic corrosion works

Galvanic corrosion happens when two different metals touch while an electrolyte, such as salt water, condensation or wet road salt, bridges them. The pair forms a battery: the more anodic metal corrodes faster than it would on its own, and the more cathodic metal corrodes slower.

Three conditions all have to be present:

- **Two metals far enough apart in the galvanic series** (or a metal and a conductive non-metal such as carbon fiber or graphite)
- **Electrical contact** between them, directly or through a fastener, bracket or ground strap
- **An electrolyte** wetting both metals at the joint

Remove any one of the three and galvanic corrosion stops. Every fix below works by breaking one of them, and the electrolyte is usually the hardest to control, which is why the same joint can last decades indoors and fail in a season on a boat.

## Galvanic series in seawater

The galvanic series ranks metals by their corrosion potential in a specific electrolyte, here flowing seawater. Metals higher in the list are more anodic and corrode when coupled to anything below them. The wider the gap between two metals, the stronger the driving force. Potentials are approximate, measured against a saturated calomel electrode (SCE).

| Metal or alloy | Approximate potential (V vs SCE) | Position |
| --- | --- | --- |
| Magnesium and magnesium alloys | -1.60 to -1.63 | Most anodic |
| Zinc (including galvanizing and zinc plate) | -0.98 to -1.03 | Anodic |
| Aluminum alloys | -0.76 to -1.00 | Anodic |
| Cadmium | -0.70 to -0.73 | Anodic |
| Mild steel, cast iron | -0.60 to -0.72 | Anodic |
| Low-alloy steel | -0.58 to -0.62 | Anodic |
| Stainless steel 410, 430 (active) | -0.46 to -0.58 | Anodic |
| Stainless steel 304 (active, in crevices) | -0.46 to -0.58 | Anodic |
| Stainless steel 316 (active, in crevices) | -0.43 to -0.54 | Anodic |
| Aluminum bronze | -0.31 to -0.42 | Middle |
| Yellow brass, naval brass, red brass | -0.30 to -0.40 | Middle |
| Tin | -0.31 to -0.33 | Middle |
| Copper | -0.30 to -0.37 | Middle |
| Lead-tin solder | -0.28 to -0.37 | Middle |
| Admiralty brass, aluminum brass | -0.28 to -0.36 | Middle |
| Manganese bronze | -0.27 to -0.34 | Middle |
| Silicon bronze | -0.26 to -0.29 | Middle |
| Copper-nickel 90/10 | -0.21 to -0.28 | Middle |
| Copper-nickel 70/30 | -0.18 to -0.23 | Middle |
| Lead | -0.19 to -0.25 | Middle |
| Nickel 200 | -0.10 to -0.20 | Cathodic |
| Silver | -0.09 to -0.14 | Cathodic |
| Stainless steel 304 (passive) | -0.05 to -0.10 | Cathodic |
| Nickel-copper alloy 400 (Monel 400) | -0.04 to -0.14 | Cathodic |
| Stainless steel 316 (passive) | 0.00 to -0.10 | Cathodic |
| Titanium and titanium alloys | -0.05 to +0.06 | Cathodic |
| Nickel-chromium-molybdenum alloy C (Hastelloy C) | -0.03 to +0.08 | Cathodic |
| Platinum | +0.19 to +0.25 | Cathodic |
| Graphite, carbon fiber composite | +0.20 to +0.30 | Most cathodic |

*Approximate ranges from the classic seawater galvanic series data presented in ASTM G82 and corrosion handbooks (flowing seawater at about 2.4 to 4 m/s, 10 to 27 C). Stainless steels appear twice: in their normal passive state and in their active state, which occurs in oxygen-starved crevices. The series changes in other electrolytes, at other temperatures and with surface condition, so treat it as a ranking, not a design calculation.*

## Allowable potential difference by environment

Galvanic compatibility tables in the style of MIL-STD-889 and similar aerospace and electronics practice group metals by an anodic index and set a limit on the difference between two metals in contact. A widely used rule of thumb looks like this:

| Service environment | Typical maximum difference for unprotected contact | Examples |
| --- | --- | --- |
| Harsh: outdoors, marine, salt spray, high humidity | About 0.15 V | Boat hardware, vehicle underbodies, coastal enclosures |
| Normal: indoors, unconditioned, occasional condensation | About 0.25 V | Warehouses, garages, unheated equipment rooms |
| Controlled: temperature and humidity controlled | About 0.50 V | Offices, labs, sealed electronics enclosures |

*A planning guide, not a guarantee. Pairs beyond these limits can still work with isolation, sealing or coatings, and pairs within them can still corrode if the anode is very small relative to the cathode.*

## Common metal pairs and what to do about them

Potential differences below are estimated from the seawater series above. Risk assumes direct contact with no isolation.

| Pair | Approximate potential difference | Corrodes | Typical risk | What to do |
| --- | --- | --- | --- | --- |
| Aluminum part, 304 or 316 stainless fasteners | About 0.6-0.9 V | Aluminum (around the fastener) | Low indoors and dry; moderate to high outdoors or in salt | Small cathode in a large anode is the favorable case, so it is widely used. Outdoors, install fasteners with a barrier compound or sealant, add isolation washers, and keep the anodize or coating intact under the head. |
| Aluminum part, carbon fiber composite | About 1.0-1.3 V | Aluminum | High wherever moisture can reach the joint | One of the worst common pairs, and the composite is often the larger area. Put a glass fiber ply or film barrier between them, seal the edges, and use titanium or suitably coated fasteners. |
| Aluminum part, copper or brass part or fitting | About 0.4-0.7 V | Aluminum | High when wet | Isolate with a nonconductive gasket, bushing or dielectric union. Avoid copper-bearing runoff onto aluminum, which can pit it even without direct contact. |
| Aluminum part, titanium fasteners or parts | About 0.7-1.0 V | Aluminum | Moderate to high when wet | Common in aerospace with anodized or primed aluminum and fasteners installed wet with sealant. Do not rely on bare contact outdoors. |
| Steel part, zinc plate or galvanizing | About 0.3-0.4 V | Zinc (by design) | Low; this is how zinc protects steel | The zinc corrodes sacrificially and protects scratches and cut edges. Coating life shortens in salt and when the zinc is coupled to a large area of stainless or copper. |
| Carbon steel part, 304 or 316 stainless fasteners | About 0.5-0.7 V | Carbon steel | Low to moderate | Small stainless fasteners in a large painted or coated steel part are usually acceptable. Keep the steel coated around the fastener. |
| Stainless part, carbon steel or zinc-plated fasteners | About 0.5-0.7 V (steel), about 0.9-1.0 V (zinc) | The fasteners | High when wet | The unfavorable area ratio: small anodes in a large cathode. Fasteners rust or lose their plating quickly outdoors. Use stainless fasteners in stainless parts. |
| Aluminum part, zinc-plated steel fasteners | About 0-0.25 V | Usually the zinc, slowly | Low | A well-matched pair. Once the zinc is consumed the steel underneath is the cathode, so in harsh service the joint still benefits from a barrier compound. |
| 304 with 316 stainless | Under about 0.1 V | Negligible | Low | Compatible. Mixing 304 fasteners with 316 parts, or the reverse, is not a galvanic concern. |

*Risk ratings are typical engineering judgments for unprotected joints. For aerospace, defense and marine work, follow the contract's dissimilar-metals requirement, often MIL-STD-889.*

## The area ratio rule

The relative size of the two metals matters as much as the potential difference. The corrosion current is spread over the anode, so:

- **Small anode, large cathode: bad.** The current concentrates on a small area. Steel rivets in a copper sheet, or carbon steel bolts in a stainless panel, corrode quickly.
- **Large anode, small cathode: usually tolerable.** The same current is spread thin. Stainless screws in an aluminum panel are the everyday example, and they last well in most indoor and many outdoor uses.

This has a counterintuitive consequence for coatings. If you paint only the anode, every scratch or pinhole becomes a tiny anode facing a large bare cathode, and corrosion there can be faster than if you had painted nothing. **When you can coat only one metal, coat the cathode, or coat both.**

A practical rule: make fasteners and other small parts the more cathodic (noble) metal, rather than the more anodic one.

## How to prevent galvanic corrosion

Each fix breaks one of the three conditions. In harsh environments, designers usually stack two or three.

**Choose compatible metals.** The simplest fix. Use fasteners and hardware close to the base metal in the series, or more cathodic and small. Stainless fasteners in stainless parts, aluminum or zinc-plated fasteners in aluminum where strength allows, titanium with carbon fiber.

**Isolate the joint.** Break electrical contact with nonconductive washers, shoulder bushings or sleeves around the fastener shank, and gaskets or tape between faying surfaces. Isolation has to cover the bolt shank and threads as well as the head, or the fastener still contacts the bore. Note that isolation can conflict with electrical grounding or bonding requirements; resolve that on the drawing.

**Keep the electrolyte out.** Seal faying surfaces and fastener holes with a sealant or a barrier compound, install fasteners wet, and design the joint to drain rather than trap water. Crevices that hold moisture also switch stainless steel into its active state.

**Coat the cathode, or both.** Paint, powder coat or primer on the cathodic metal shrinks the effective cathode area. See the area ratio rule above.

**Pick finishes that help.** [Anodizing](/reference/anodizing-spec) puts an electrically insulating oxide on aluminum, which helps at broad faying surfaces, though it is scraped through at threads and under fastener heads, so it is not a complete isolator on its own. [Zinc plating](/blog/zinc-plating) on steel fasteners brings them close to aluminum in the series. Chromate or trivalent conversion coatings on aluminum and zinc improve corrosion resistance and give paint a good base.

**Add a sacrificial anode.** On boats, tanks and buried structures, a zinc, aluminum or magnesium anode bolted to the structure corrodes in its place. This is a system design choice rather than a part-level fix.

## Aluminum with carbon fiber and titanium

These two pairs come up constantly in drones, bikes, motorsport and aerospace parts, and they behave differently.

[Carbon fiber](/materials/carbon-fiber) composite is electrically conductive and sits at the cathodic end of the series, near graphite. Bonded or bolted directly to aluminum in a wet environment, it drives rapid corrosion of the aluminum, often hidden under the joint until it fails. The standard practice is a layer of glass fiber or an insulating film at the interface, sealed edges, and titanium or coated fasteners rather than bare aluminum or steel.

Titanium sits close to carbon fiber and to passive stainless steel in the series, so titanium fasteners in carbon fiber are a compatible pair. Titanium against aluminum is not: the aluminum is the anode, and outdoors the joint needs the same sealing and isolation as stainless fasteners in aluminum. For more on choosing between the two metals, see [titanium vs aluminum](/blog/titanium-vs-aluminum).

## How to prevent rust on steel parts

Rust is the corrosion of iron and steel into iron oxide when oxygen and moisture are present. It is not galvanic corrosion, though dissimilar-metal contact can speed it up. The main options for a steel part, roughly from lightest to heaviest protection:

- **Oil or wax** after machining, for parts that will be painted later or used indoors
- **[Black oxide](/reference/black-oxide-spec)** plus oil, for mild indoor protection with almost no dimensional change
- **[Zinc plating](/blog/zinc-plating)** with a passivate, for general hardware and indoor or sheltered outdoor use
- **[Powder coating](/reference/powder-coating-spec)** or paint over a pretreatment, for durable color and outdoor service
- **Hot-dip galvanizing**, for structural steel and heavy outdoor exposure
- **A stainless steel**, when coatings are impractical, with [passivation](/reference/passivation-spec) to remove free iron left on the surface by machining

Design helps as much as finish: avoid pockets and crevices that trap water, provide drain holes in tubes and enclosures, and keep dissimilar-metal fasteners isolated.

## What to put on the drawing

Shops can only protect a joint they know about. When a part will be in contact with a different metal, say so:

- The mating material and fastener material, if the shop is supplying hardware
- The finish by specification, for example anodize per MIL-A-8625 Type II or zinc plating per ASTM B633 with thickness class
- Masking requirements, such as bare aluminum at a grounding point or no anodize in a bore
- Any isolation hardware, sealant or wet-install requirement, and the governing standard if there is one

Upload the part with those notes at [openspindle.com/quote](/quote). The matched shop quotes the part, the finish and any hardware together.

Potentials and compatibility ratings are approximate and environment dependent. For aerospace, defense and marine parts, the dissimilar-metals requirement in your contract or specification governs.

## On OpenSpindle

- [Anodizing spec](https://openspindle.com/reference/anodizing-spec.md)
- [Zinc plating](https://openspindle.com/blog/zinc-plating.md)
- [Titanium vs aluminum](https://openspindle.com/blog/titanium-vs-aluminum.md)
- [Carbon fiber](https://openspindle.com/materials/carbon-fiber.md)
- [Passivation spec](https://openspindle.com/reference/passivation-spec.md)
- [Metal properties comparison](https://openspindle.com/reference/metal-properties-comparison.md)
- [Thread galling](https://openspindle.com/blog/thread-galling.md)

## Frequently asked questions

### What is galvanic corrosion?

Galvanic corrosion is accelerated corrosion of one metal when it is in electrical contact with a more cathodic metal and both are wetted by an electrolyte such as salt water or condensation. The more anodic metal, for example aluminum against stainless steel, corrodes faster than it would alone.

### Can you use stainless steel screws in aluminum?

Yes, in most indoor and many outdoor uses, because the small stainless fastener in a large aluminum part is a favorable area ratio. In marine, salt or constantly wet service, install the screws with a barrier compound or sealant, use isolation washers, and keep the anodize or coating intact around the hole.

### Does carbon fiber cause galvanic corrosion with aluminum?

Yes. Carbon fiber is conductive and strongly cathodic to aluminum, so a wet joint between them corrodes the aluminum quickly. Separate the two with a glass fiber ply or insulating film, seal the edges, and use titanium or coated fasteners.

### Which metals are galvanically compatible?

Metals close together in the galvanic series, such as 304 and 316 stainless, titanium and passive stainless, or aluminum and zinc, are generally compatible. Common guidance limits the potential difference to about 0.15 V in harsh outdoor or marine service, 0.25 V indoors without climate control, and 0.50 V in controlled environments.

### Does anodizing prevent galvanic corrosion?

It helps but is not a complete fix. Anodize is an electrical insulator, so it reduces galvanic current across broad faying surfaces, but fasteners scrape through it at threads and under heads. In harsh service, combine anodize with a sealant or barrier compound and isolation washers.

### What is MIL-STD-889?

MIL-STD-889 is the US Department of Defense standard on dissimilar metals. It groups metals by galvanic compatibility and sets requirements for protecting dissimilar-metal joints in military hardware, and it is widely referenced as a galvanic compatibility guide outside defense work too.