Materials

Inconel 625 vs 718: How to Choose

Both are nickel superalloys with similar price. The choice comes down to whether you need corrosion and weldability (625) or heat-treated strength (718).

Tom PetriniCo-founder, OpenSpindle
Published 6 min read
Inconel 625 vs 718: How to Choose

The short answer

Inconel 625 is a solid-solution Ni-Cr-Mo alloy with excellent corrosion resistance, good weldability, and moderate strength up to 650 °C. Inconel 718 is a precipitation-hardening Ni-Cr-Fe-Nb alloy that trades a little corrosion resistance for roughly twice the yield strength when aged. Specify 625 for chemical, marine, and welded aerospace structure; specify 718 for turbine disks, high-strength fasteners, and aerospace parts that will see mechanical load at temperature.

The property comparison

Both are nickel superalloys and shops that run one almost always run the other. The real difference is heat treatability: 625 is solid-solution strengthened (no significant heat treatment response), while 718 is precipitation-hardenable and gets most of its strength from a solution-treat and age cycle.

PropertyInconel 625Inconel 718
Yield strength (annealed)~60 ksi~65 ksi
Yield strength (aged)No age response~140 ksi
Tensile strength (aged)~120 ksi~180 ksi
Density8.44 g/cm³8.19 g/cm³
Max service temperature~980 °C (short term)~700 °C (sustained)
WeldabilityExcellent, no PWHT requiredWeldable, prone to strain-age cracking
Corrosion (seawater, chlorides)ExcellentGood
MachinabilityPoor (Ni superalloy)Poor (Ni superalloy)
Typical cost (bar, per lb)BaselineRoughly similar

When 625 wins

Choose Inconel 625 for chemical-process components, marine and offshore hardware, flue-gas desulfurization, and anywhere corrosion resistance plus weldability is the hard requirement. The alloy welds beautifully with matching ERNiCrMo-3 filler and typically needs no post-weld heat treatment, which is why it dominates aerospace welded assemblies, exhaust components, and chemical reactors. It also has strong oxidation resistance up to about 980 °C short-term, so it covers moderate high-temperature service without needing an age cycle.

When 718 wins

Choose Inconel 718 for turbine disks, blades, high-strength fasteners, aerospace structural brackets, and anything that will see mechanical stress at temperature. Age-hardened 718 reaches 140 ksi yield and 180 ksi tensile, more than twice annealed 625, and it holds that strength well up to about 650 °C. It is the default aerospace superalloy for strength-driven applications. The downside is welding: 718 is prone to strain-age cracking in the heat-affected zone, so welding typically needs full re-solution and age heat treatment to restore properties and relieve stress.

Machining both of them

Neither is pleasant to machine. Both work-harden aggressively; both demand carbide tooling with positive geometry, modest SFM (typically 50-150 depending on operation), rigid setup, and tool paths that keep the cutter engaged. The practical difference: 718 is machined solution-annealed and age-hardened after, which means two machining passes (rough-mill, age-harden, finish-mill) for parts that need tight dimensions after heat treat. 625 is machined to final dimension in one setup. Factor the extra pass into 718 cost estimates.

Cost realities

Per pound, 625 and 718 are usually within 10 percent of each other at the mill level. On a finished part, 718 often costs more because of the two-pass machining and the heat treat cycle required to develop its strength. If a design will work in annealed 625, specifying 718 adds cost without benefit; conversely, specifying 625 for a part that will see sustained mechanical stress at 500 °C will fail. Pick by the dominant requirement, not habit.

The quick decision rule

If the design is driven by corrosion resistance, chemical compatibility, or will involve welding without post-weld heat treatment, use 625. If the design is driven by mechanical strength, especially at elevated temperature or in a rotating component, use 718. If both drive the design (some aerospace applications), the usual answer is 718 with careful attention to the welding and heat treatment plan. For anything else, name the specific property you need and let the alloy follow.

Where to source

OpenSpindle routes nickel-superalloy RFQs to shops with the rigid machines, carbide tooling library, and heat-treatment partners to handle both grades. AS9100 and NADCAP shops are available where the end use requires them. See the Inconel material page for grades and properties, or send a drawing for a quote.

Last reviewed by Tom Petrini

Let us quote your next part.

Upload your CAD or drawing and tell us your budget. We source it across our global network of partner shops and come back with your best-match quote, typically within about 24 hours.

  • Free quote in about 24 hours
  • No minimum order